We did it! It was an intense 3 weeks at this cob workshop we held at the end of September and beginning of October in Castelo Branco.
12 students from different backgrounds came together on this land to learn, hands-on, how to build an earthen structure. We had some nice sunny days and a beautiful red clay to build this cob sauna from the ground up, with beautiful earthen plasters and a tadelakt shower, a green reciprocal roof on top, and a funnel-like wattle and daub structure at the skylight to diffuse light and keep the sauna insulated.
Lots of creativity, flexibility and good fun! See some pictures of the process, and the tadelakt recipe to try on your own building.












Clay soil, sand, straw and water: the materials we used to build this project. We started with the earthen floor, so the first layer could dry while we began the base for the walls.
As the walls went up, we started integrating elements: windows, niches and shelves, sculptures, and whatever other ideas came up while we built. There is a design, but we transform some aspects as we go.




While we build, we also make sure the walls remain plumb, to keep a proper building style and save material. The cob wall gets a bit thinner toward the top: every meter, it loses 5 cm in thickness. This makes the wall more stable by reducing the weight on top.
As we build, we can integrate bottles and pieces of wood as anchors for the roof.




Tadelakt
This polishing compacts the surface and closes the pores. Once finished, it should be left to rest for no more than 24 hours.
A natural soap is then applied and the surface is polished again. This soap is typically made from olive oil, and the fats it contains react chemically with the lime to form a calcium soap, known as calcium oleate, which creates a water-repellent film, resulting in a glossy, smooth and very hard finish.
It is a very meticulous technique, as the lime dries quickly, and if you take your eye off it for even a moment, it may start to set, at which point it will be too late to continue polishing or to apply the soap. For this very reason, it is very important to maintain a suitable working environment, paying attention to the humidity and keeping the layers moist to control the drying process.
It is important to understand that this technique requires lime with specific characteristics: traditionally, Marrakech lime is used, which contains natural impurities that give it mild hydraulic properties, ideal for polishing. These impurities include silica, alumina and clay. Furthermore, it is fired using traditional methods, resulting in a unique finish.
Today, adaptations have been developed using natural hydraulic limes (NHL 2 or NHL 3.5), depending on local availability, or also using lime putty prepared from non-hydraulic lime. The key is to understand that the process requires the right lime, meticulous polishing, and the application of soap to achieve water repellency.
















Leave it to rest and cure for 8 to 16 hours before applying the soap.
You may notice that, after this time, water appears on the surface, known as ‘lime sweat’. This must be removed with a cloth before applying the soap and proceeding to the second stage of polishing.
Apply the soap with a sponge, after diluting it in water, and polish again with a stone. This can be repeated 3 to 5 times, until a white streak appears, which indicates that the wall is no longer absorbing it.
The Tadelakt is ready! It must be left to cure for at least 2 weeks, after which beeswax can be applied to seal it. Beeswax should be diluted in olive oil, 1 part of beeswax to 3 parts of oil.
To apply it, follow these steps:
The base coat must be a properly applied and smoothed lime render, in a ratio of 1:3 (lime : sand), which must be moistened repeatedly before work begins.
The Tadelakt mixture is applied in two coats, each 2 mm thick.
The first coat must be applied firmly to ensure adhesion, leaving it well smoothed and levelled with a floating trowel.
It is left to dry briefly, until it reaches the ‘leather-hard’ or ‘partially set’ stage: the surface is firm but the interior is still damp.
Apply the second coat, repeating the same procedure.
Leave it to dry until polishing can begin. This is done using hard stones (6 to 10 on the Moh scale). To determine when to start, the stone should not retain any traces of the mixture when rubbed over the surface. Polish vigorously, using continuous circular movements, until the pores are sealed.




CONTACT US
tierramigo@gmail.com
If you would like to request more information about workshops, if you would like to host one, or information regarding consultancy, please contact us and we'll get back to you as soon as possible.
In the subject line, please indicate whether your message is about workshops, consultations, training, projects, or other.